Ceramics · Practical application guide
Ceramics. Color & firing trials.
Keep clay-body, engobe and glaze trials separate, and assess iron oxide only after the complete firing and cooling cycle.

Choose the layer before choosing a percentage
In fired ceramics, pigment can enter the clay body, an engobe or a glaze. The percentage must identify that layer’s dry basis. A cement roof tile cures chemically; a clay roof tile passes through a kiln. Successful cold-cured concrete color does not establish the same fired shade or ceramic suitability.
Mason Color’s reference guide distinguishes body-stain suitability and explains that composition, firing cycle, atmosphere and cooling affect color. Treat its temperature notes as grade-specific guidance, not a general firing temperature for FUXIN iron oxides. Ceramic grade and firing guidance
Calculate from dry material, not water-containing clay
If the ceramic technologist has selected a 2% addition on dry body, 1,000 g dry clay body receives 20 g colorant. This percentage is a calculation example, not a universal body-stain recommendation. Do not subtract the colorant from the base unless the approved formula explicitly requires replacement.
| Material being weighed | Dry basis for the example | Colorant at the selected 2% |
|---|---|---|
| Dry body powder | 1,000 g | 20 g |
| 1,250 g moist clay with verified 20% water by wet mass | 1,000 g | 20 g |
| Incorrect calculation on all 1,250 g wet clay | 1,250 g assumed | 25 g, too much for this target |
The moisture figure must be measured or documented for the material. A slip or glaze suspension also needs its dry-solids content established before calculating colorant addition. Write whether the recipe means addition to 100 parts base or a percentage of the final total; those are not mathematically identical.
Use a separate glaze experiment when appropriate
Glendale Community College’s ceramics teaching reference discusses iron-oxide additions across 0.5–6% in oxidation glazes, with different results in reduction. This is educational glaze context, not a recipe for roof-tile bodies and not a color guarantee. Iron-oxide glaze reference
If your ceramic specialist confirms the selected oxide and stable base glaze are suitable, a proposed comparison can use 100 g dry base glaze with 0, 1, 2 and 4 g colorant. These are additions on base weight, producing totals of 100, 101, 102 and 104 g before water. Keep glaze preparation and applied coating mass consistent. Do not transfer the glaze ladder to an engobe or body without separate approval.
Run a documented kiln trial
- Prepare the control and candidates with the same body, water source and mixing method. Disperse color thoroughly and use the process’s normal screening procedure. Record any retained agglomerates rather than hiding them by changing the formula.
- Form or coat identical labeled pieces. Measure a relevant dimension before firing so shrinkage can be compared. For coated samples, record application mass or thickness using the workshop’s established method.
- Dry and fire through the actual production schedule, including all required firings. Record kiln position, atmosphere, heating stages, hold and cooling; peak temperature alone is insufficient.
- Place duplicates in different documented positions to distinguish a recipe effect from kiln variation. Keep the uncolored control in the same run.
- Judge the fully cooled pieces. Compare shade with cracking, warping, glaze defects and the product’s required absorption or strength results.
Use the fired defects to choose the next trial
| Result | Check before adding more oxide |
|---|---|
| Same formula, different shelf color | Firing atmosphere and heatwork |
| Specks or streaks | Dispersion and raw-material contamination |
| Blisters or excessive flow | Base chemistry, colorant effect and firing |
| Cracked coating | Body/engobe/glaze compatibility |
| Dry powder shade does not survive firing | Colorant chemistry in the actual ceramic system |
Mason’s technical FAQ gives examples of chemistry-sensitive color changes and incompatible stain combinations. Ceramic troubleshooting context Do not chase the target only by increasing percentage. Keep dust controlled and follow material safety sheets. Send FUXIN the target fired piece, layer chemistry, dry-basis formula and kiln record to establish whether a suitable grade can be offered. Roof-tile durability and other service requirements still need finished-product evidence.
Technical references
- Mason Color Works: Ceramic reference guide
- Glendale Community College: Sources of color in glaze
- Mason Color Works: Technical FAQ
Independent technical guidance used for this application overview. These references are not FUXIN project case studies or a substitute for a grade-specific technical data sheet.