Concrete color hardener · Practical application guide
Color hardener. Mixing & coverage.
Keep the pigment percentage inside the manufactured blend separate from the kilograms of complete hardener applied per square metre.

Treat the hardener as a complete dry blend
A concrete color hardener combines pigment, cement and graded fine aggregate. Its abrasion-resistant surface depends on the complete formulation and installation, not on pigment alone. Loose iron oxide should not be broadcast as a replacement. Brickform’s technical description explicitly identifies those three material groups. Hardener composition
For FUXIN pigment selection, the manufacturer’s job is to establish the colorant level within its hardener recipe. For the installer, the main number is the application rate of the finished hardener. Keep those two calculations on separate lines of the batch or application sheet.
Calculate pigment inside the factory formulation
Suppose a development batch has 25 kg uncolored dry base containing 8 kg cement, and its already approved candidate uses 3% dry pigment on cement. The pigment addition is 240 g, giving 25.240 kg finished material if no other ingredient changes. It is not 750 g, which would result from applying 3% to the entire base.
| Development record | Example value |
|---|---|
| Uncolored binder/aggregate base | 25.000 kg |
| Cement within that base | 8.000 kg |
| Selected pigment loading | 3% of cement |
| Powder pigment added | 0.240 kg |
| Finished development blend | 25.240 kg |
This is dosage arithmetic, not a recommended hardener formulation. Preserve the validated cement and aggregate grading. If the recipe’s approved pigment basis includes other binders, count them as specified. General construction-pigment information does not establish a finished hardener’s strength or coverage. Defined pigment-dose basis
Calculate the complete hardener required for the slab
As a named-product reference, Brickform specifies a 60 lb bucket over 120 ft² for most applications, equivalent to approximately 2.44 kg/m². Its lighter-color example increases material to 60 lb over 90 ft², approximately 3.25 kg/m². These rates are for complete Brickform hardener, not pigment and not an automatic rate for another formula. Coverage data
At the first example rate, a 5 m² trial requires approximately 12.2 kg finished hardener before waste. Mark the trial area and weigh the allocation in advance. Otherwise an uneven handful-by-handful application can make a correct factory color formula appear inconsistent.
Apply a representative two-stage trial
For trained installers: follow the product SDS and specified dust-control and protective-equipment requirements before handling dry hardener.
- Use the intended concrete and finish method. Confirm readiness from surface conditions and the hardener instructions, not a universal number of minutes after the pour.
- In Brickform’s procedure, application starts after excess bleed water has disappeared. Approximately 75–80% is applied first, followed by the remaining 20–25% after wetting and floating. For a chosen 75:25 split of 12.2 kg, weigh 9.15 kg then 3.05 kg. This is the cited product’s application example. Two-stage application
- Allow the material to take up moisture and work it in using the specified float. Apply the second portion evenly, addressing thin coverage. Do not add loose color or dry cement as a patch.
- Complete the intended texture or stamping, then follow the curing and sealing system. Record the actual mass used, weather and finishing sequence.
Diagnose appearance and surface integrity
| Symptom | Check before changing pigment |
|---|---|
| Gray patches | Thin coverage or surface disruption |
| Dark finishing marks | Overworking or inconsistent tools |
| Dry, loose material | Application timing and wetting |
| Surface separation | Concrete and hardener installation conditions |
Do not judge the factory formula only from the unsealed wet slab. Retain a finished, dry trial and verify the required abrasion, bond and other surface performance. Review any defect with the complete-hardener supplier before specifying a repair. Send FUXIN the cement basis, pigment mass, hardener blend details and completed trial result when requesting a candidate grade; the pigment alone cannot certify the finished wearing surface.
Technical references
- Brickform: Color Hardener composition
- Davis Colors: Pigment product data
- Brickform: Color Hardener technical information
Independent technical guidance used for this application overview. These references are not FUXIN project case studies or a substitute for a grade-specific technical data sheet.