Dry-mix mortar · Practical application guide
Dry-mix mortar. Batching & color.
Convert an approved binder-based pigment dose into a dry-mortar batch sheet, then check discharge and packaging uniformity.

Define the percentage before weighing a tonne
A dry mortar contains binder, sand and functional additives, so “3% pigment” is incomplete unless the denominator is written down. Davis’s ready-mix concrete guidance gives typical powder dosages around 1–5% against its defined cementitious content, excluding sand; that source is not a dry-mortar prescription. Use grade-specific guidance to select your candidate; the calculations below use an already selected 3% binder-based trial, not a universal dry-mortar prescription. Reference dosage basis
Scholz identifies powder grades suited to dry mortars and highlights the application’s dispersion demands. Choose a form that your mixer can actually distribute, especially when the formulation contains cellulose, polymers or very fine fillers. Dry-mortar pigment selection
Scale the laboratory result correctly
Assume the approved uncolored dry base contains 25% reference binder. The remainder is its unchanged sand and additive package.
| Base material before pigment | Binder at 25% | Pigment at 3% of binder | Final dry mass |
|---|---|---|---|
| Laboratory: 2.000 kg | 0.500 kg | 15 g | 2.015 kg |
| Pilot: 100.000 kg | 25.000 kg | 750 g | 100.750 kg |
| Production: 1,000.000 kg | 250.000 kg | 7.500 kg | 1,007.500 kg |
This arithmetic preserves the base formulation and treats pigment as an addition. Do not silently replace cement or polymer with pigment. If packaging must contain 25.000 kg of finished dry product, normalize the formula: 25 / 1.0075 gives approximately 24.814 kg base plus 186.1 g pigment. Keep all base ingredients in their original relative proportions. This is a net-mass calculation, not approval of a formulation change.
Set up a measurable plant trial
- Confirm the microingredient scale can resolve the intended pigment dose. Weigh a check load before the trial and record the actual addition rather than only the target displayed by the controller.
- Run an uncolored control, then the selected colored formula. Keep batch fill level and the mixer cycle fixed initially. A pigment premix may improve dosing, but any carrier must come from or be accounted for in the formula.
- Inspect the complete charging route for retained color: a correct scale total does not prove all material reached the mixer. Check the hopper, transfer line and discharge after a controlled shutdown under plant safety procedures.
- Sample finished material from the beginning, middle and end of discharge. Label bags with batch and sampling position. Keep the samples separate rather than pooling away possible variation.
- Repeat the preferred process once before releasing the recipe. Lödige describes product-specific mixing and discharge requirements for mortars; there is no single published mixing time suitable for every formulation. Mixing-system context
Judge wet-mixed samples, not only dry powder
Prepare equal finished-product masses from each retained bag using the same water ratio, mixer and test age. If a chosen laboratory procedure uses 300 g water, an accidental extra 15 g changes that amount by 5%. Record such differences rather than blaming pigment immediately. The 300 g figure is an arithmetic example, not a water recommendation.
Make identical finished specimens and retain the uncolored control. Compare dry shade, specks and texture alongside the mortar’s relevant flow, working-time and hardened tests. Add a storage or transport trial when bag segregation or caking is suspected. A uniform-looking powder is insufficient evidence of uniform finished color.
Find the process step causing variation
| Pattern in the results | Investigate | Action to verify |
|---|---|---|
| Early bags differ from late bags | Discharge segregation or retained material | Repeat position-based sampling |
| Every bag contains specks | Incomplete pigment dispersion | Change one mixing variable |
| One entire batch differs | Wrong addition, source or water in testing | Audit its batch record |
| Stored bags differ from fresh | Moisture ingress or handling | Test retained sealed samples |
Keep an accepted dried panel, master recipe revision and incoming pigment lot reference together. SPEC MIX describes controlled weighing and preblending as central to factory-colored mortar consistency. Factory color-control example Send FUXIN the binder basis, required pigment mass per batch, mixer type and observed dispersion results for a production-focused sample request.
Technical references
- Davis Colors: Construction dosage basis
- Scholz: Mortars and plasters
- Lödige: Building-material mixing
- SPEC MIX: Factory colored mortar
Independent technical guidance used for this application overview. These references are not FUXIN project case studies or a substitute for a grade-specific technical data sheet.