Plastics · Practical application guide
Plastics. Loading & processing.
Work out what reaches the polymer, calibrate the feeder, and qualify color through the actual thermal and forming history.

Use a product-specific starting point
Record the resin grade, virgin/recycled ratio, molding or extrusion route, wall thickness and end use. Decide whether you will add dry powder, masterbatch or a precolored compound. A masterbatch’s addition rate is not its pigment concentration. Its carrier and other additives also enter the finished material; match them to the polymer before choosing a convenient feeder setting.
As a real manufacturer example, Avient’s Colorant Chromatics PEI bulletin lists 2% for 680.00 black but 15% for 680.02 red. Those rates concern particular PEI masterbatches, not FUXIN iron oxide or a generic black/red recipe. The contrast shows why one let-down percentage should not be applied across grades. The bulletin labels these as LDR addition rates without explicitly defining the denominator; the following mass calculations are independent examples, not an interpretation of that table. Avient PEI product-specific rates
Calculate on final blend or host resin explicitly
For a stated 2% of final blend, a calculated 10.00 kg batch is 0.20 kg masterbatch + 9.80 kg other formula components. If those other components are only natural resin, that is the complete weighing split. If the instruction instead means 2 parts masterbatch per 100 parts host resin, 10.00 kg host needs 0.20 kg masterbatch, and the resulting blend is 10.20 kg. Masterbatch is then 1.961% of the blend. Clarify the supplier’s denominator rather than treating these conventions as identical.
For an actual pigment fraction c in a masterbatch, final pigment fraction = masterbatch fraction × c. Do not infer c from pellet color or a nominal color name.
Worked pigment-equivalent comparison
The following is a calculated training example, not an asserted Avient composition or a recommended loading range. Assume a compatible concentrate is documented as 40% pigment and you are comparing already-approved candidate additions in a 10 kg final blend. The balance must retain the intended host/additive formulation.
| Concentrate/final blend | Concentrate | Pigment delivered | Carrier/other concentrate material |
|---|---|---|---|
| 1% | 100 g | 40 g (0.4%) | 60 g |
| 2% | 200 g | 80 g (0.8%) | 120 g |
| 3% | 300 g | 120 g (1.2%) | 180 g |
To target 0.8% pigment with a different concentrate containing 20% pigment, the arithmetic requires 0.008 ÷ 0.20 = 4% concentrate. Equal pigment mass does not establish equal shade, dispersion, carrier compatibility or finished-part properties.
Calibrate, compound and form
- Retain an approved-color or uncolored control from the same resin lot. Dry the resin and concentrate only as their respective instructions require.
- Calibrate and verify feeder output using the equipment manufacturer’s procedure, including any specified catch-weigh method. Compare verified addition with the required mass ratio; do not rely solely on the dial. Avient’s linked guidance supports choosing equipment suited to the colorant form. Avient feeding guidance
- Keep the resin/additive package constant while screening the colorant. Record actual melt temperature, throughput, screw settings and residence-time changes.
- Collect plaques or extrudate after the process stabilizes. Label start-up and post-stop material separately. Use identical thickness, texture and backing for color comparisons.
- Repeat the intended second melt-processing pass if the product undergoes one. Inspect the final article rather than declaring success from compounded pellets.
Test heat stability with the real history
Treat temperature, time, polymer and pigment concentration as a combined test condition. LANXESS distinguishes engineered yellow iron oxide and zinc-ferrite grades in its heat-stable range; that does not assign the same limit to ordinary yellow or to another manufacturer’s grade. Heat-stable grade distinctions
Compare normal-run specimens with specimens from the longest approved residence time, without exceeding the resin or pigment limits. Use the same formula for both. Record color change and physical defects separately; a retained color does not prove the polymer has avoided degradation.
Troubleshooting and finished-product release
| Problem | First checks | Controlled next step |
|---|---|---|
| Specks | Dispersion, contamination, feeder bridging | Inspect concentrate and a thin specimen |
| Run-to-run shade drift | Actual dosing, resin/recycle lot, thickness | Repeat with weighed feed and fixed material |
| Discoloration after stoppage | Residence and thermal history | Compare approved stop/restart specimens |
| Warp or surface change | Carrier, additives, processing | Test actual part against the control |
Use appropriate ISO 23900 dispersion methods, such as filter-pressure or film assessment, where applicable. Keep test conditions aligned. Check dimensions, mechanical properties and required aging alongside color. Filter-pressure scope; Film-test scope
Prepare the technical inquiry
Send FUXIN the polymer grade, target plaque, thickness, loading denominator, masterbatch pigment fraction if known, thermal history and trial results. Include the delivery form and tests required for the finished article. This lets a grade comparison focus on reproducible color and processing evidence.
Technical references
- Avient: Colorant Chromatics PEI Masterbatch product bulletin (2020)
- Avient — Avoid these three mistakes to get the most from color
- LANXESS — Heat stable inorganic yellow pigments
- ISO — ISO 23900-5:2015: filter pressure value test
- ISO — ISO 23900-6:2015: film test
Independent technical guidance used for this application overview. These references are not FUXIN project case studies or a substitute for a grade-specific technical data sheet.