Rubber · Practical application guide
Rubber. phr, color & cure.
Translate pigment targets into weigh-outs, account for the carrier rubber, and compare dispersion and cure before releasing a color.

Keep rubber phr separate from compound percentage
phr means parts by mass per hundred parts of rubber. Fillers, oil and pigment are not normally part of that reference rubber mass. A stated 2 phr pigment is therefore not 2% of a filled compound. Write the elastomer basis, cure type and colorant delivery form at the top of the trial sheet. Use the compounder’s approved definition when polymer-bearing concentrates are present.
Start from a qualified neutral compound. There is no defensible universal iron-oxide loading for all EPDM, SBR, NBR and silicone articles. Select the actual color trial window from the qualified formula or grade instructions, then use the calculations below to weigh it accurately.
A real concentrate example and its limitation
Akrochem describes Akrosperse color masterbatches as approximately 50% pigment, in elastomer carriers including SBR and EPR. Its chart includes oxide-red products as well as other pigment chemistries. The approximate concentration is not a batch assay; obtain the actual pigment and carrier fractions for precise substitution. Akrochem concentrate composition
The carrier is functional material. Akrochem explains that an unsuitable SBR carrier can change the cure behavior of low-unsaturation rubbers such as EPDM. Matching the pigment color does not establish carrier compatibility. Rubber-carrier interactions
Worked powder-to-masterbatch balance
Calculated example only: the qualified target is assumed to be 2 phr active pigment on 10.00 kg total elastomer. A documented 50% pigment/50% compatible-rubber concentrate would require 200 g pigment ÷ 0.50 = 400 g concentrate. It also supplies 200 g carrier rubber. To retain 10.00 kg total elastomer, the separately charged base rubber becomes 9.80 kg. This substitution still requires the compounder’s approval.
| Weigh-out option | Separate base rubber | Dry pigment | 50/50 color concentrate | Total elastomer |
|---|---|---|---|---|
| Powder route | 10,000 g | 200 g | 0 g | 10,000 g |
| Concentrate route | 9,800 g | 0 g | 400 g | 10,000 g |
The powder route assumes the weighed material is the defined pigment without a separate carrier; diluted powder preparations need their own composition correction. Other approved ingredients remain calculated on the same total-elastomer basis. Do not subtract the carrier from filler, or count the full concentrate as rubber. If the concentrate contains oil or processing aids, use its actual composition rather than this simplified 50/50 model. Adding 400 g concentrate to 10 kg rubber without adjustment makes 10.2 kg elastomer: 200/10,200 × 100 = 1.961 phr, with the rest of the formulation also shifted relative to total rubber.
Build the trial without changing the cure blindly
- Prepare the approved control and candidate formulations on paper, including carrier accounting. Keep raw-material lots and total-elastomer basis comparable.
- Follow the validated mixer sequence. Establish pigment addition where enough shear is available for incorporation; do not improvise the curative addition stage. Color compounding guidance
- Record mixer loading, time and actual stock temperature. Compare handling with the control and inspect a representative sheet or cut section for specks.
- Sheet and cool according to the established procedure before storage. Keep batches traceable; avoid uncontrolled hot stacking. Rubber color handling
- Measure the candidate cure curve before molding the final article. If it changes, investigate carrier and ingredients with the compounder; do not simply increase sulfur or peroxide.
- Cure representative parts using the approved schedule. Compare conditioned pieces, because an uncured stock match is not the final color.
Make the cure and color checks comparable
Use the same rotorless cure-meter method, instrument and conditions for the reference and candidate. Review scorch behavior, cure time and torque response against the plant’s established specification. ASTM D5289 notes that instrument designs can give different responses, so an unrelated supplier curve is not an equivalent baseline. Cure-meter comparison
Measure cured color on matched surface texture and thickness. Check the article’s specified hardness, tensile/elongation, compression-set or aging performance as applicable. Include contact-staining or bloom assessment when relevant. A visually better red is not a release decision if the cure or part properties fail.
Troubleshooting and silicone boundary
| Observation | Check first | Next step |
|---|---|---|
| Streaks or colored dots | Addition point and available shear | Compare a compatible predispersed form |
| Cure curve shifts | Carrier composition and rubber balance | Hold release; review the complete compound |
| Surface bloom or staining | Oil/additives, pigment form, cure | Run the relevant conditioned contact test |
| Color differs after cure | Cure history and base-compound shade | Compare identically cured reference parts |
Silicone needs its own compatible color preparation and cure/metering route. Do not transfer these conventional-rubber mixing instructions to liquid silicone. Silicone-specific color preparation
Make the inquiry reproducible
Send FUXIN the elastomer and cure system, active-pigment phr target, colorant composition, carrier balance, cure curves and cured reference part. Ask for a grade trial tied to those conditions and retain the selected compound’s full release record.
Technical references
- Akrochem: Masterbatch Color Properties, approximately 50% pigment and carrier options
- Akrochem: Dispersions of Color Pigments, rubber-carrier compatibility
- Akrochem — Compounding colored rubber articles
- Akrochem — Color chart for rubber and compounding suggestions
- ASTM International — ASTM D5289-19a(2026): rubber vulcanization using rotorless cure meters
- Dow — XIAMETER CP Series Color Masterbatch
Independent technical guidance used for this application overview. These references are not FUXIN project case studies or a substitute for a grade-specific technical data sheet.