Keep the qualified UHPC formula as the baseline
Start with a UHPC system already qualified for the component. Pigment is a formulation change to evaluate with the same mixer, fiber system and curing route. The NPCA 2026 architectural UHPC guide addresses solid and liquid pigments and the need to test their effect on the matrix. It does not provide one transferable FUXIN dosage. UHPC pigment and batching guidance
The tables below are calculation examples at 1%, 2% and 3%, not a recommended UHPC trial window. Use only levels accepted for your actual system. Preserve an unpigmented control and keep every water or admixture adjustment visible as a separate trial.
Do not confuse the two percentage denominators
If a test contains 12 kg qualifying cementitious material within 24 kg total dry premix, 240 g dry pigment is 2% of binder but 1% of total dry premix. Both statements describe the same mass. A source limit expressed on dry materials cannot be applied as though it used binder mass.
| Calculation only | Dry pigment for 12 kg binder | Rate against 24 kg dry premix |
|---|---|---|
| 1% of binder | 120 g | 0.5% |
| 2% of binder | 240 g | 1.0% |
| 3% of binder | 360 g | 1.5% |
Here the dry-premix denominator is defined before pigment addition. State that convention in the record. Proprietary bag mass is not automatically cementitious mass; use the disclosed binder content or the supplier’s explicit premix-basis instruction. Do not replace cement with the calculated pigment.
Account for liquid color by actual composition
Liquid color mass = required dry pigment ÷ dry-pigment mass fraction. Water contribution equals liquid mass × verified water fraction. In this arithmetic example only, a suspension contains 60% pigment and 40% water; actual products may contain other solids or carriers.
| Dry-pigment target | Example suspension required | Water carried into batch |
|---|---|---|
| 120 g | 200 g | 80 g |
| 240 g | 400 g | 160 g |
| 360 g | 600 g | 240 g |
For the 240 g target, 160 g carrier water belongs in the existing batch-water budget. Do not add it on top and then call the formula unchanged. Re-homogenize the suspension before weighing. Liquid-color water accounting
Use a staged mixing record
- Record the starting material temperatures, mixer identity, load and time zero. Weigh pigment and each liquid independently.
- Use the UHPC system’s qualified charging sequence. NPCA’s described route introduces dry materials, then water/liquid superplasticizer, and fibers after fluidization; verify the pigment insertion point within that route. Manufacturing sequence
- At the agreed checkpoints, record elapsed time, temperature and the chosen flow measurement. Use the same test method and timing for baseline and colored batches.
- Keep the established fiber-addition and placement procedure. Photograph flow into a representative thin edge or relief, and inspect for fiber clusters and voids.
- If flow or temperature leaves the qualified range, stop and investigate. Do not restore a visual result with undocumented water.
Check the actual geometry and cure
FHWA notes that UHPC mixing energy, placement-dependent fiber behavior and curing affect performance. UHPC production background Make a component-like specimen and the required test specimens from the same trial. Record any thermal treatment as a complete cycle; this page assigns no generic pigment heat limit. Compare the finished dry face after the planned surface processing, and repeat the selected batch before release.
Troubleshooting and release
| Observation | Check first | Next action |
|---|---|---|
| Flow lower than baseline | Pigment mass, water ledger and dispersion | Repeat under controlled batching; review a revised formula |
| Excess fluidity with liquid color | Carrier water counted twice or omitted | Correct the water calculation |
| Temperature rises faster | Load, cycle and material temperature | Review mixer procedure and system limits |
| Fiber-rich marks or weak interfaces | Placement route and fiber distribution | Investigate and test representative pieces |
| Good color but failed properties | Unqualified formulation change | Reject the color recipe pending reformulation |
Send FUXIN and the UHPC supplier the dry sample, exact denominator, liquid composition if used, flow/temperature records and test results. Release the combination only when appearance and specified UHPC performance both pass.
Technical references
- NPCA: Guide to Manufacturing Architectural Precast UHPC Elements, 2026
- FHWA: UHPC Materials and Production