Stamped concrete · Practical application guide
Stamped concrete. Pigment & two-tone trials.
Calculate the base-color dose from cementitious mass, then test the release color and sealer as separate appearance variables.

Choose integral color or a complete surface hardener
For integral color, pigment enters the concrete mix and its dose follows the specified cementitious reference mass. A dry-shake hardener is a separate manufactured binder-and-aggregate product applied at a surface coverage rate. Decide which route is being used before calculating material. Loose oxide powder cannot stand in for either a complete color hardener or a stamp-release product.
Solomon’s dry-integral-color sheet identifies a 2–4% total-cementitious reference range for its ready-mix colors. An initial 3% candidate lies within that named-product window, but FUXIN grade suitability and the project concrete must still be established by samples. Integral-color reference
Calculate by concrete batch, not by square metre
Assume the approved project needs 6 m³ concrete containing 320 kg reference cementitious material per m³, and its selected pigment dose is 3%. These are hypothetical project inputs, not a slab design.
Pigment = volume × cementitious content × dose fraction. The total is 6 × 320 × 0.03 = 57.6 kg dry pigment.
| Delivery or trial | Concrete volume | Binder mass | Pigment at 3% |
|---|---|---|---|
| First delivery | 4 m³ | 1,280 kg | 38.4 kg |
| Second delivery | 2 m³ | 640 kg | 19.2 kg |
| Combined | 6 m³ | 1,920 kg | 57.6 kg |
If the second mix has different cementitious content, recalculate its pigment and make a matching sample. Equal pigment kilograms per truck do not preserve the ratio when truck volume changes. Record powder grade and actual mass on each batch ticket; do not convert slurry to powder kilogram-for-kilogram.
Separate base color from release highlights
A colored release powder both prevents sticking and creates an antiquing effect; a clear liquid release performs release without the same colored-powder contribution. Brickform documents these distinct functions. Colored release; Clear release
Make a small comparison matrix rather than changing everything at once. For example, test base candidate A with the chosen release, then base candidate B with that same release. Next, compare an alternative release on the preferred base. Keep the stamp, texture depth and finishing route consistent. Do not improvise a release agent by mixing loose iron oxide into an arbitrary liquid.
Build the sample through the entire work sequence
- Use the actual concrete ingredients and target consistency. Include the planned stamp pattern, border and joint detail in a representative trial. Do not add extra water to make wet color look closer to the reference.
- Mix the integral pigment by the validated route for its form and packaging. Ordinary bags must be emptied; only packaging explicitly designed for incorporation can enter a mixer.
- Place and finish the trial, then stamp when the concrete is ready for the selected tooling and release system. Use surface condition rather than an invented universal elapsed time.
- Clean release residue by the product’s approved method at the required stage. Keep the cleaning procedure identical across comparison panels.
- Apply the intended cure/seal system and assess the dry result. Label an unsealed reference if useful, but approve the appearance that will actually be delivered.
Diagnose the layer responsible for a mismatch
| Appearance | Investigate first |
|---|---|
| Entire panel too light | Base recipe, pigment mass, water and drying |
| Recesses too dark | Release selection and residue removal |
| Glossy patches | Sealer distribution and surface preparation |
| Gray surface marks | Finishing damage or thin hardener coverage |
| Poor wet traction | Complete texture/sealer system |
A base pigment change cannot reliably fix excess antiquing residue or uneven sealer. Evaluate wet appearance and the required traction separately; stamping texture alone does not prove slip resistance. Retain the fully finished panel and the recorded recipe. Send FUXIN the target base color, cementitious content and sample findings when requesting the pigment quantity and grade for production.
Technical references
- Solomon Colors: Dry Integral Colors specifications
- Brickform: Antique Release
- Brickform: Liquid Release
- Brickform: Concrete design guide
Independent technical guidance used for this application overview. These references are not FUXIN project case studies or a substitute for a grade-specific technical data sheet.